How to Measure Carburized Case Depth Using a Microhardness Gradient

20 11,2026
Laizhou Jincheng Industrial Equipment Co.,Ltd
JCTEST explains how to measure the hardened case depth of carburized and quenched steel using a microhardness gradient, including test-point placement and depth criteria.

Carburized and quenched steel typically has a hard surface layer and a lower-hardness core. A microhardness gradient shows how hardness changes with distance from the surface and can be used to determine the effective case depth when a hardness threshold has been specified.

For laboratories and manufacturers, a reliable result depends on more than the hardness tester. The cross-section, preserved surface edge, test-point placement and acceptance criterion must all suit the inspection requirement.

What does effective case depth mean?

Effective case depth is the distance from the relevant surface to the location where hardness reaches a specified limiting value. It is not necessarily the same as the total depth affected by carburizing, which may be assessed using different criteria.

Define the criterion before testing: agree on the applicable standard, hardness threshold, test method, measurement location and any drawing or customer requirements. Do not apply a threshold from another specification without checking that it is appropriate.

How to establish a microhardness gradient

  1. Select the inspection location. Identify the functional surface and the section specified for the component. Record the location and orientation so the result can be related to the part and repeated when needed.
  2. Prepare a representative cross-section. Cut the sample with care to avoid significant heat damage. Mount it when necessary to support the edge, then grind and polish the cross-section so that indentations can be measured clearly. Preserve the original surface and avoid edge rounding or excessive removal.
  3. Set the test conditions. Select the microhardness method, test force and dwell time in accordance with the applicable standard and inspection requirements. Check the tester, indenter and measuring system using the appropriate verification procedure and reference materials.
  4. Place the test points. Measure distances from the relevant original surface into the cross-section, normally along a line perpendicular to that surface. Choose positions that characterize the gradient and bracket the specified threshold. Maintain the indentation-to-edge and indentation-to-indentation spacing required by the applicable procedure; a staggered pattern may be used where appropriate.
  5. Measure and record. Record the hardness and corresponding depth for each indentation, together with the test conditions. Plotting hardness against depth makes the transition toward the core easier to assess.
  6. Determine the effective case depth. Identify where the hardness profile reaches the specified threshold. If the governing procedure permits interpolation between points, use the points that bracket the threshold. Report the result using the required method and units.

Test-point placement and preparation: practical checks

  • Near-surface measurements: the first indentation must be close enough to characterize the case but sufficiently far from the edge to satisfy the applicable spacing rules. A damaged or rounded edge can make the depth reference unreliable.
  • Threshold region: plan enough points around the expected transition to locate the threshold. If the initial points do not bracket it, consider additional measurements where the procedure and available space allow.
  • Surface condition: scratches, relief, deformation or unclear indentation corners can affect hardness readings. Review preparation quality before attributing an unusual gradient to heat treatment.
  • Curved or complex parts: define the measurement location and surface reference according to the inspection requirement. Local geometry can affect both preparation and the direction in which depth is measured.

Interpreting and reporting the result

A hardness gradient should be assessed against the specified threshold and acceptance limits, not against a generic case-depth value. If readings are irregular, review sample preparation, point placement, indentation measurements and equipment verification before drawing a conclusion. The component itself may also have local variations that require further investigation.

If the measured profile does not reach or bracket the threshold within the tested region, a threshold-based depth cannot be established from those points alone. Do not extrapolate or declare a pass or failure without following the applicable reporting and acceptance rules.

Include in the test record

  • Sample identification, inspection location and surface reference
  • Applicable standard or procedure and specified hardness threshold
  • Test method, force, dwell time and equipment verification details
  • Individual depths and hardness readings, including any interpolation used
  • Calculated case depth, acceptance criterion and relevant observations

Choosing equipment for the workflow

The workflow combines cross-section preparation with microhardness testing and indentation measurement. Equipment selection should reflect the material, expected case depth, component geometry, applicable standard, sample volume and any need for automated measurement or data output. Specifications and supported functions should be confirmed against the technical documentation for the selected model.

JCTEST supplies materials testing equipment and solutions. To discuss a suitable setup, share the component details, inspection standard, required threshold and expected workload via WhatsApp or visit www.jctesthardness.com.

Name *
Email *
Message *

Recommended Products

Popular articles
Recommended Reading

Related Reading

Contact us
Contact us
https://shmuker.oss-accelerate.aliyuncs.com/tmp/temporary/60ec5bd7f8d5a86c84ef79f2/60ec5bdcf8d5a86c84ef7a9a/thumb-prev.png